Pit-type furnace gas nitriding process operation
Leave a message
Principles for Preparatory Treatment:
1. Quenching and tempering is used for general structural steel parts. The high-temperature tempering temperature should be 20-40°C higher than the nitriding temperature, and the holding time should not be too long.
2. Normalizing can be used for parts with low impact toughness requirements, but the cooling rate during normalizing should be rapid. Normalizing should not be used for parts with larger cross-sectional dimensions.
3. 38CrMoAl steel should be quenched and tempered, otherwise needle-shaped nitrides will easily form in the nitrided layer. Tool and die steel must be quenched and tempered before nitriding; annealing is not permitted.
4. For slender, thin-walled, complex, and precision parts, one or more stress relief treatments are required before nitriding. The stress relief temperature is generally lower than the quenching and tempering temperature but higher than the nitriding temperature. If deformation exceeds tolerance after treatment, correct the deformation and then stress relieve again according to the original process until the deformation is completely within acceptable limits.
Preparatory Work:
1. Equipment Preparation
1) Before nitriding, thoroughly inspect the temperature control instrumentation, liquid ammonia cylinder, flowmeter, ammonia decomposition meter, and various piping systems to ensure proper operation of the equipment. The temperature difference within the furnace should be less than 10°C.
2) Desiccants such as calcium oxide and calcium chloride are commonly used. Calcinated calcium oxide is often used. If it fails, it should be replaced or dried.
3) The volume fraction of water used in the nitriding medium should preferably be less than 0.2% liquid ammonia.
4) Prepare the lifting equipment based on the part's shape, size, quality, and technical requirements. Before use, carefully inspect the components for integrity and ensure they are secure and clean.
2. Part Preparation
1) The surface roughness of nitriding parts must be Ra 1.6μm or less. Surface defects such as burrs, dents, and rust must be avoided. Parts that cannot be processed promptly must be oiled to prevent rust.
2) For parts prone to deformation, the amount of deformation should be estimated and recorded.
3) The material and pre-heat treatment of the specimens should be the same as the parts. Specimen dimensions should be 20-30 mm x 6-10 mm. Three to five specimens should be numbered and placed in representative locations.
4) Carefully clean the parts. Before hoisting them into the furnace, wipe them clean with clean gasoline to ensure cleanliness.
5) Load the cleaned parts into the nitriding furnace. For slender rods prone to deformation, they must be hung vertically with uniform spacing. Do not block the exhaust holes. Parts must not exceed the effective heating zone.
Determination of Process Specifications:
1. Nitriding Temperature
1) 500-530°C is commonly used to ensure a high dispersion of nitrides and high hardness.
2) As the nitriding temperature increases, the depth of the nitrided layer increases, while the hardness decreases significantly. Nitriding temperatures above 550°C result in hardnesses below 1000 HV for most steel grades.
3) When using two-stage or three-stage nitriding, the temperature of the second stage is usually below 560°C.
2. Nitriding Time
1) The nitrided layer thickens with increasing nitriding time. The initial growth rate is rapid, then gradually slows, following a parabolic curve. The rate is generally around 0.01 mm/h.
2) As the holding time increases, the nitrides aggregate and grow, and the hardness decreases. The higher the temperature and the longer the holding time, the greater the growth.
3. Ammonia Decomposition Rate
1) An ammonia decomposition rate of 25%-40% is optimal, as active nitrogen atoms are maximized, leading to significant nitrogen absorption on the part surface.
2) When the ammonia decomposition rate exceeds 60%, the hydrogen volume fraction in the atmosphere reaches 52%, resulting in a denitrification effect. A large number of nitrogen and hydrogen molecules remain on the part surface, preventing nitrogen atoms from being absorbed and thinning the nitrided layer.
3) For one-stage or two-stage nitriding, an ammonia decomposition rate of 18%-30% for strong nitriding and 40%-60% for diffusion nitriding is ideal.
Nitriding Operation:
1. Heating: Before heating, ammonia should be introduced for exhaust gas flow. The ammonia flow rate should be at least twice the normal operating flow rate. For applications with strict deformation requirements, a step-by-step heating method should be used, with holding times of 1-2 hours at 200-250°C and 400-450°C. A heating rate of less than 50°C/hour is also acceptable. As the holding time approaches, the amount of ammonia should be increased to keep the decomposition rate within the process requirements.
2. Venting: Venting is generally performed while heating, within a temperature range of 150-200°C. During the venting process, the furnace and piping seals can be checked using pH test paper (soaked in water, it turns blue when exposed to ammonia) or a glass rod (a glass rod dipped in salt emits white smoke when exposed to ammonia).
During the venting phase, ammonia is continuously introduced to maintain a pressure of 200-400 Pa. Because ammonia is readily soluble in water, the U-shaped tube used to measure the ammonia decomposition rate is typically filled with oil. In the nitriding tank, the air is kept clear, and the vent pipe cannot be ignited. During the heating phase, the ammonia decomposition rate can reach 70%. When the ammonia volume fraction in the furnace gas exceeds 95%, the ammonia flow rate can be reduced to maintain a positive pressure in the furnace.
3. Holding: After the temperature reaches the specified process temperature, adjust the ammonia flow rate to maintain an ammonia decomposition rate between 18% and 35%, and begin the holding time. The furnace pressure should be between 200 and 600 Pa. During the nitriding process, the ammonia flow rate is adjusted to control the ammonia decomposition rate. The rate is generally measured every 15 to 30 minutes. During the holding process, the furnace temperature should fluctuate within 5°C. Near the end of the holding period, samples should be removed from the sampling port for necessary analysis.
4. Denitrification Cooling: After the nitriding phase is complete, close the exhaust valve, reduce the ammonia flow rate, and hold for 2 hours to maintain an ammonia decomposition rate above 70%. This will lower the nitrogen concentration on the part surface and reduce surface brittleness. Afterwards, power off the furnace to cool it down, but continue to introduce a small amount of ammonia gas to maintain positive pressure. Ammonia supply can be discontinued once the furnace temperature drops below 150°C. Parts should be removed from the furnace to avoid collision.